| Physical Properties | Metric | English | Comments | ||
|---|---|---|---|---|---|
| Density | 1.30 g/cc | 0.0470 lb/in³ | |||
| 1.46 g/cc | 0.0527 lb/in³ | DAM; ISO 1183 | |||
| Water Absorption | 5.0 % @Thickness 2.00 mm |
5.0 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 | ||
| Moisture Absorption | 1.50 % @Thickness 2.00 mm |
1.50 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 | ||
| Viscosity | 69730 cP @Shear Rate 5000 1/s, Temperature 300 °C |
69730 cP @Shear Rate 5000 1/s, Temperature 572 °F |
ISO 11403-1 -2 | ||
| 92504 cP @Shear Rate 5000 1/s, Temperature 290 °C |
92504 cP @Shear Rate 5000 1/s, Temperature 554 °F |
ISO 11403-1 -2 | |||
| 127400 cP @Shear Rate 5000 1/s, Temperature 280 °C |
127400 cP @Shear Rate 5000 1/s, Temperature 536 °F |
ISO 11403-1 -2 | |||
| 318080 cP @Shear Rate 500 1/s, Temperature 300 °C |
318080 cP @Shear Rate 500 1/s, Temperature 572 °F |
ISO 11403-1 -2 | |||
| 438400 cP @Shear Rate 500 1/s, Temperature 290 °C |
438400 cP @Shear Rate 500 1/s, Temperature 554 °F |
ISO 11403-1 -2 | |||
| 615000 cP @Shear Rate 500 1/s, Temperature 280 °C |
615000 cP @Shear Rate 500 1/s, Temperature 536 °F |
ISO 11403-1 -2 | |||
| Viscosity Test | 130 cm³/g | 130 cm³/g | DAM; ISO 307 1157 1628 | ||
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm | 0.0030 in/in | DAM; ISO 294-4 2577 | ||
| Linear Mold Shrinkage, Transverse | 0.0070 cm/cm | 0.0070 in/in | DAM; ISO 294-4 2577 | ||
| Mechanical Properties | Metric | English | Comments | ||
| Tensile Strength at Break | 110 MPa | 16000 psi | 50%RH; ISO 527-1/-2 | ||
| 145 MPa | 21000 psi | DAM; ISO 527-1/-2 | |||
| Tensile Stress | 9.12 MPa @Strain 0.230 %, Temperature 90.0 °C |
1320 psi @Strain 0.230 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | ||
| 10.3 MPa @Strain 0.410 %, Temperature 150 °C |
1490 psi @Strain 0.410 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |||
| 11.92 MPa @Strain 0.390 %, Temperature 150 °C |
1729 psi @Strain 0.390 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |||
| 13.89 MPa @Strain 0.560 %, Temperature 180 °C |
2015 psi @Strain 0.560 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |||
| 17.77 MPa @Strain 0.370 %, Temperature 90.0 °C |
2577 psi @Strain 0.370 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |||
| 18.46 MPa @Strain 0.240 %, Temperature 23.0 °C |
2677 psi @Strain 0.240 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 24.88 MPa @Strain 0.440 %, Temperature 40.0 °C |
3609 psi @Strain 0.440 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 25.55 MPa @Strain 1.53 %, Temperature 150 °C |
3706 psi @Strain 1.53 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |||
| 28.83 MPa @Strain 0.930 %, Temperature 90.0 °C |
4181 psi @Strain 0.930 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |||
| 28.98 MPa @Strain 1.80 %, Temperature 180 °C |
4203 psi @Strain 1.80 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |||
| 30.54 MPa @Strain 1.40 %, Temperature 150 °C |
4429 psi @Strain 1.40 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |||
| 33.2 MPa @Strain 2.68 %, Temperature 150 °C |
4820 psi @Strain 2.68 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |||
| 36.61 MPa @Strain 3.06 %, Temperature 180 °C |
5310 psi @Strain 3.06 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |||
| 37.55 MPa @Strain 3.99 %, Temperature 150 °C |
5446 psi @Strain 3.99 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |||
| 37.6 MPa @Strain 0.930 %, Temperature 90.0 °C |
5450 psi @Strain 0.930 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |||
| 40.07 MPa @Strain 2.35 %, Temperature 150 °C |
5812 psi @Strain 2.35 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |||
| 40.99 MPa @Strain 1.71 %, Temperature 90.0 °C |
5945 psi @Strain 1.71 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |||
| 41.45 MPa @Strain 4.41 %, Temperature 180 °C |
6012 psi @Strain 4.41 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |||
| 43.89 MPa @Strain 0.900 %, Temperature 40.0 °C |
6366 psi @Strain 0.900 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 46.09 MPa @Strain 0.480 %, Temperature 0.000 °C |
6685 psi @Strain 0.480 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 46.66 MPa @Strain 3.50 %, Temperature 150 °C |
6767 psi @Strain 3.50 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |||
| 48.39 MPa @Strain 2.71 %, Temperature 90.0 °C |
7018 psi @Strain 2.71 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |||
| 51.91 MPa @Strain 1.51 %, Temperature 90.0 °C |
7529 psi @Strain 1.51 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |||
| 56.04 MPa @Strain 0.580 %, Temperature -20.0 °C |
8128 psi @Strain 0.580 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 56.38 MPa @Strain 0.620 %, Temperature 0.000 °C |
8177 psi @Strain 0.620 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 59.41 MPa @Strain 1.39 %, Temperature 40.0 °C |
8617 psi @Strain 1.39 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 60.48 MPa @Strain 0.910 %, Temperature 23.0 °C |
8772 psi @Strain 0.910 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 62.79 MPa @Strain 0.710 %, Temperature 40.0 °C |
9107 psi @Strain 0.710 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 63.34 MPa @Strain 2.22 %, Temperature 90.0 °C |
9187 psi @Strain 2.22 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |||
| 70.92 MPa @Strain 0.780 %, Temperature 23.0 °C |
10290 psi @Strain 0.780 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 71.24 MPa @Strain 0.760 %, Temperature -20.0 °C |
10330 psi @Strain 0.760 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 71.32 MPa @Strain 1.99 %, Temperature 40.0 °C |
10340 psi @Strain 1.99 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 77.68 MPa @Strain 0.860 %, Temperature 0.000 °C |
11270 psi @Strain 0.860 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 77.99 MPa @Strain 1.30 %, Temperature 23.0 °C |
11310 psi @Strain 1.30 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 83.91 MPa @Strain 1.00 %, Temperature 40.0 °C |
12170 psi @Strain 1.00 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 89.13 MPa @Strain 0.960 %, Temperature -20.0 °C |
12930 psi @Strain 0.960 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 93.57 MPa @Strain 1.79 %, Temperature 23.0 °C |
13570 psi @Strain 1.79 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 98.89 MPa @Strain 1.13 %, Temperature 0.000 °C |
14340 psi @Strain 1.13 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 102.34 MPa @Strain 1.21 %, Temperature 23.0 °C |
14843 psi @Strain 1.21 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 104.57 MPa @Strain 1.35 %, Temperature 40.0 °C |
15167 psi @Strain 1.35 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 105.98 MPa @Strain 1.31 %, Temperature 0.000 °C |
15371 psi @Strain 1.31 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 113.5 MPa @Strain 1.29 %, Temperature -20.0 °C |
16460 psi @Strain 1.29 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 122.88 MPa @Strain 1.79 %, Temperature 40.0 °C |
17822 psi @Strain 1.79 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 123.75 MPa @Strain 1.50 %, Temperature 0.000 °C |
17948 psi @Strain 1.50 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 124.19 MPa @Strain 1.59 %, Temperature 23.0 °C |
18012 psi @Strain 1.59 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 124.89 MPa @Strain 1.73 %, Temperature 0.000 °C |
18114 psi @Strain 1.73 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 134.88 MPa @Strain 1.58 %, Temperature -20.0 °C |
19563 psi @Strain 1.58 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 137.07 MPa @Strain 1.69 %, Temperature -20.0 °C |
19880 psi @Strain 1.69 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 142.25 MPa @Strain 2.05 %, Temperature 23.0 °C |
20632 psi @Strain 2.05 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 146.77 MPa @Strain 1.93 %, Temperature 0.000 °C |
21287 psi @Strain 1.93 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 159.71 MPa @Strain 2.04 %, Temperature -20.0 °C |
23164 psi @Strain 2.04 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 180.18 MPa @Strain 2.58 %, Temperature -20.0 °C |
26133 psi @Strain 2.58 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 10.0 MPa @Strain 0.160 %, Time 360000 sec |
1450 psi @Strain 0.160 %, Time 100 hour |
50%RH; isochronous; ISO 11403-1 -2 | |||
| 10.0 MPa @Strain 0.170 %, Time 3.60e+6 sec |
1450 psi @Strain 0.170 %, Time 1000 hour |
50%RH; isochronous; ISO 11403-1 -2 | |||
| 10.0 MPa @Strain 0.140 %, Time 3600 sec |
1450 psi @Strain 0.140 %, Time 1.00 hour |
50%RH; isochronous; ISO 11403-1 -2 | |||
| 10.0 MPa @Strain 0.150 %, Time 36000 sec |
1450 psi @Strain 0.150 %, Time 10.0 hour |
50%RH; isochronous; ISO 11403-1 -2 | |||
| Elongation at Break | 2.5 % | 2.5 % | DAM; ISO 527-1/-2 | ||
| 2.6 % | 2.6 % | 50%RH; ISO 527-1/-2 | |||
| Tensile Modulus | 7.80 GPa | 1130 ksi | 50%RH; ISO 527-1/-2 | ||
| 8.80 GPa | 1280 ksi | DAM; ISO 527-1/-2 | |||
| 2.343 GPa @Temperature 150 °C |
339.8 ksi @Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |||
| 2.383 GPa @Temperature 170 °C |
345.6 ksi @Temperature 338 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 2.60 GPa @Temperature 170 °C |
377 ksi @Temperature 338 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 2.865 GPa @Temperature 150 °C |
415.5 ksi @Temperature 302 °F |
DAM; ISO 11403-1 -2 | |||
| 3.164 GPa @Temperature 110 °C |
458.9 ksi @Temperature 230 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 3.85 GPa @Temperature 110 °C |
558 ksi @Temperature 230 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 4.501 GPa @Temperature 60.0 °C |
652.8 ksi @Temperature 140 °F |
50%RH; ISO 11403-1 -2 | |||
| 7.371 GPa @Temperature 60.0 °C |
1069 ksi @Temperature 140 °F |
DAM; ISO 11403-1 -2 | |||
| 7.863 GPa @Temperature 30.0 °C |
1140 ksi @Temperature 86.0 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 7.974 GPa @Temperature 30.0 °C |
1157 ksi @Temperature 86.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 8.223 GPa @Temperature -20.0 °C |
1193 ksi @Temperature -4.00 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 8.911 GPa @Temperature -70.0 °C |
1292 ksi @Temperature -94.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 9.102 GPa @Temperature -20.0 °C |
1320 ksi @Temperature -4.00 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 9.311 GPa @Temperature -100 °C |
1350 ksi @Temperature -148 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 9.975 GPa @Temperature -20.0 °C |
1447 ksi @Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 10.062 GPa @Temperature -70.0 °C |
1459.4 ksi @Temperature -94.0 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 10.237 GPa @Temperature -20.0 °C |
1484.8 ksi @Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 10.491 GPa @Temperature -100 °C |
1521.6 ksi @Temperature -148 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| Shear Modulus | 1.297 GPa @Temperature 100 °C |
188.1 ksi @Temperature 212 °F |
50%RH; Dynamic; ISO 11403-1 -2 | ||
| 1.604 GPa @Temperature 100 °C |
232.6 ksi @Temperature 212 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 1.87 GPa @Temperature 60.0 °C |
271 ksi @Temperature 140 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 2.637 GPa @Temperature 60.0 °C |
382.5 ksi @Temperature 140 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 3.02 GPa @Temperature 10.0 °C |
438 ksi @Temperature 50.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 3.138 GPa @Temperature -40.0 °C |
455.1 ksi @Temperature -40.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 3.253 GPa @Temperature 10.0 °C |
471.8 ksi @Temperature 50.0 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 3.331 GPa @Temperature -70.0 °C |
483.1 ksi @Temperature -94.0 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 3.469 GPa @Temperature -100 °C |
503.1 ksi @Temperature -148 °F |
DAM; Dynamic; ISO 11403-1 -2 | |||
| 3.485 GPa @Temperature -40.0 °C |
505.5 ksi @Temperature -40.0 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 3.754 GPa @Temperature -70.0 °C |
544.5 ksi @Temperature -94.0 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| 3.915 GPa @Temperature -100 °C |
567.8 ksi @Temperature -148 °F |
50%RH; Dynamic; ISO 11403-1 -2 | |||
| Secant Modulus | 0.516 GPa @Strain 8.09 %, Temperature 200 °C |
74.9 ksi @Strain 8.09 %, Temperature 392 °F |
DAM; ISO 11403-1 -2 | ||
| 0.660 GPa @Strain 5.90 %, Temperature 200 °C |
95.8 ksi @Strain 5.90 %, Temperature 392 °F |
DAM; ISO 11403-1 -2 | |||
| 0.887 GPa @Strain 3.88 %, Temperature 200 °C |
129 ksi @Strain 3.88 %, Temperature 392 °F |
DAM; ISO 11403-1 -2 | |||
| 1.33 GPa @Strain 1.99 %, Temperature 200 °C |
193 ksi @Strain 1.99 %, Temperature 392 °F |
DAM; ISO 11403-1 -2 | |||
| 2.14 GPa @Strain 0.640 %, Temperature 200 °C |
311 ksi @Strain 0.640 %, Temperature 392 °F |
DAM; ISO 11403-1 -2 | |||
| 2.87 GPa @Strain 2.62 %, Temperature 40.0 °C |
416 ksi @Strain 2.62 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 4.04 GPa @Strain 1.58 %, Temperature 40.0 °C |
587 ksi @Strain 1.58 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 4.32 GPa @Strain 2.29 %, Temperature 23.0 °C |
627 ksi @Strain 2.29 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 4.88 GPa @Strain 0.900 %, Temperature 40.0 °C |
707 ksi @Strain 0.900 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 5.65 GPa @Strain 2.28 %, Temperature 40.0 °C |
820 ksi @Strain 2.28 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 5.65 GPa @Strain 0.440 %, Temperature 40.0 °C |
820 ksi @Strain 0.440 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |||
| 5.76 GPa @Strain 1.45 %, Temperature 23.0 °C |
835 ksi @Strain 1.45 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 6.35 GPa @Strain 2.11 %, Temperature 0.000 °C |
921 ksi @Strain 2.11 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 6.65 GPa @Strain 0.910 %, Temperature 23.0 °C |
964 ksi @Strain 0.910 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 6.99 GPa @Strain 2.28 %, Temperature 0.000 °C |
1010 ksi @Strain 2.28 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 7.5027 GPa @Strain 1.48 %, Temperature 40.0 °C |
1088.2 ksi @Strain 1.48 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 7.5578 GPa @Strain 1.73 %, Temperature 23.0 °C |
1096.2 ksi @Strain 1.73 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 7.58 GPa @Strain 1.99 %, Temperature -20.0 °C |
1100 ksi @Strain 1.99 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 7.60 GPa @Strain 2.20 %, Temperature -20.0 °C |
1100 ksi @Strain 2.20 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 7.69 GPa @Strain 0.240 %, Temperature 23.0 °C |
1120 ksi @Strain 0.240 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 7.87 GPa @Strain 1.43 %, Temperature 0.000 °C |
1140 ksi @Strain 1.43 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 8.04 GPa @Strain 1.64 %, Temperature 0.000 °C |
1170 ksi @Strain 1.64 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 8.391 GPa @Strain 1.00 %, Temperature 40.0 °C |
1217 ksi @Strain 1.00 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 8.46 GPa @Strain 1.21 %, Temperature 23.0 °C |
1230 ksi @Strain 1.21 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 8.54 GPa @Strain 1.58 %, Temperature -20.0 °C |
1240 ksi @Strain 1.58 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 8.61 GPa @Strain 1.41 %, Temperature -20.0 °C |
1250 ksi @Strain 1.41 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 8.75 GPa @Strain 1.13 %, Temperature 0.000 °C |
1270 ksi @Strain 1.13 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 8.84 GPa @Strain 0.710 %, Temperature 40.0 °C |
1280 ksi @Strain 0.710 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |||
| 9.03 GPa @Strain 0.860 %, Temperature 0.000 °C |
1310 ksi @Strain 0.860 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 9.09 GPa @Strain 0.780 %, Temperature 23.0 °C |
1320 ksi @Strain 0.780 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |||
| 9.09 GPa @Strain 0.620 %, Temperature 0.000 °C |
1320 ksi @Strain 0.620 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |||
| 9.28 GPa @Strain 0.960 %, Temperature -20.0 °C |
1350 ksi @Strain 0.960 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| 9.37 GPa @Strain 0.760 %, Temperature -20.0 °C |
1360 ksi @Strain 0.760 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |||
| 9.60 GPa @Strain 0.480 %, Temperature 0.000 °C |
1390 ksi @Strain 0.480 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |||
| 9.66 GPa @Strain 0.580 %, Temperature -20.0 °C |
1400 ksi @Strain 0.580 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |||
| Charpy Impact Unnotched | 4.10 J/cm² | 19.5 ft-lb/in² | DAM; ISO 179/1eU | ||
| 4.10 J/cm² | 19.5 ft-lb/in² | 50%RH; ISO 179/1eU | |||
| 4.00 J/cm² @Temperature -30.0 °C |
19.0 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU | |||
| 4.00 J/cm² @Temperature -30.0 °C |
19.0 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU | |||
| Charpy Impact, Notched | 0.400 J/cm² | 1.90 ft-lb/in² | DAM; ISO 179/1eA | ||
| 0.400 J/cm² | 1.90 ft-lb/in² | 50%RH; ISO 179/1eA | |||
| 0.300 J/cm² @Temperature -30.0 °C |
1.43 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA | |||
| 0.400 J/cm² @Temperature -30.0 °C |
1.90 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA | |||
| Tensile Creep Modulus, 1 hour | 5290 MPa @Pressure 55.0 MPa, Temperature 23.0 °C |
767000 psi @Pressure 7980 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | ||
| 5380 MPa @Pressure 50.0 MPa, Temperature 23.0 °C |
781000 psi @Pressure 7250 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 5638 MPa @Pressure 40.0 MPa, Temperature 23.0 °C |
817700 psi @Pressure 5800 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 6000 MPa @Pressure 30.0 MPa, Temperature 23.0 °C |
870000 psi @Pressure 4350 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 6510 MPa @Pressure 20.0 MPa, Temperature 23.0 °C |
944000 psi @Pressure 2900 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 7140 MPa @Pressure 10.0 MPa, Temperature 23.0 °C |
1.04e+6 psi @Pressure 1450 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 7000 MPa @Time 3600 sec |
1.02e+6 psi @Time 1.00 hour |
50%RH; ISO 899-1 | |||
| Tensile Creep Modulus, 1000 hours | 3793.1 MPa @Pressure 55.0 MPa, Temperature 23.0 °C |
550140 psi @Pressure 7980 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | ||
| 3920 MPa @Pressure 50.0 MPa, Temperature 23.0 °C |
569000 psi @Pressure 7250 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 4280 MPa @Pressure 40.0 MPa, Temperature 23.0 °C |
620000 psi @Pressure 5800 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 4761.9 MPa @Pressure 30.0 MPa, Temperature 23.0 °C |
690660 psi @Pressure 4350 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 5320 MPa @Pressure 20.0 MPa, Temperature 23.0 °C |
772000 psi @Pressure 2900 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 5880 MPa @Pressure 10.0 MPa, Temperature 23.0 °C |
853000 psi @Pressure 1450 psi, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |||
| 6000 MPa @Time 3.60e+6 sec |
870000 psi @Time 1000 hour |
50%RH; ISO 899-1 | |||
| Electrical Properties | Metric | English | Comments | ||
| Volume Resistivity | 2.00e+12 ohm-cm | 2.00e+12 ohm-cm | 50%RH; IEC 60093 | ||
| 8.00e+14 ohm-cm | 8.00e+14 ohm-cm | DAM; IEC 60093 | |||
| Surface Resistance | 3.00e+14 ohm | 3.00e+14 ohm | 50%RH; IEC 60093 | ||
| Dielectric Strength | 41.0 kV/mm | 1040 kV/in | DAM; IEC 60243-1 | ||
| 41.0 kV/mm | 1040 kV/in | 50%RH; IEC 60243-1 | |||
| Thermal Properties | Metric | English | Comments | ||
| CTE, linear, Parallel to Flow | 23.0 µm/m-°C | 12.8 µin/in-°F | DAM; ISO 11359-1/-2 | ||
| CTE, linear, Transverse to Flow | 60.0 µm/m-°C | 33.3 µin/in-°F | DAM; ISO 11359-1/-2 | ||
| Specific Heat Capacity | 2.28 J/g-°C | 0.545 BTU/lb-°F | |||
| Thermal Conductivity | 0.260 W/m-K | 1.80 BTU-in/hr-ft²-°F | of melt | ||
| Melting Point | 245 °C | 473 °F | DAM; 10°C/min; ISO 11357-1/-3 | ||
| Deflection Temperature at 1.8 MPa (264 psi) | 230 °C | 446 °F | DAM; ISO 75-1/-2 | ||
| Glass Transition Temp, Tg | 90.0 °C | 194 °F | DAM; 10°C/min; ISO 11357-1/-2 | ||
| Flammability, UL94 | HB @Thickness 1.50 mm |
HB @Thickness 0.0591 in |
DAM; IEC 60695-11-10 | ||
| De |
|||||
| Delivery form | Pellets | ||||
| Processing | Injection Moulding | ||||
| Regional Availability | Europe | ||||
| Near East/Africa | |||||
| Special characteristics | Heat stabilised or stable to heat | ||||
概述
PA塑料(尼龍,聚酰胺),英文名稱:Polyamide
PA的品種繁多,有PA6、PA66、PAll、PAl2、PA46、PA610、PA612、PAl010等,以及近幾年開發的半芳香族尼龍PA6T和特種尼龍等很多新品種。
物理性能
比重:PA6 1.14克/立方厘米,PA66 1.15克/立方厘米,PA1010 1.05克/立方厘米
成型收縮率:PA6 0.8-2.5% ,PA66 1.5-2.2%
成型溫度:220-300℃
干燥條件:100-110℃/12小時
堅韌、耐磨、耐油、,耐水、抗酶菌、但吸水大
燃燒鑒別方法:火焰上端黃色,下端藍色,燃燒后塑料熔滴落,起泡,離火后特殊的羊毛,指甲燒焦味和帶芹菜味
|
尼龍6: |
彈性好,沖擊強度,吸水較大 |
|
尼龍66: |
性能優于尼龍6,強度高,耐磨性好 |
|
尼龍610: |
與尼龍66相似,但吸水小,剛度低 |
|
尼龍1010: |
半透明,吸水小。耐寒性較好。適于制作一般機械零件、減磨耐磨零件、傳動零件以及化工、電器、儀表等零件 |
成型性能
1、結晶料,熔點較高,熔融溫度范圍窄,熱穩定性差,料溫超過300度、滯留時間超過30分鐘即分解。較易吸濕,需干燥,含水量不得超過0.3%。
2、流動性好,易溢料。宜用自鎖時噴嘴,并應加熱。
3、成型收縮范圍及收縮率大,方向性明顯,易發生縮孔、變形等。
4、模溫按塑件壁厚在20~90度范圍內選取,注射壓力按注射機類型、料溫、塑件形狀尺寸、模具澆注系統選定,成型周期按塑件壁厚選定。樹脂粘度小時,注射、冷卻時間應取長,并用白油作脫模劑。
5、模具澆注系統的形式和尺寸,增大流道和澆口尺寸可減少縮水。
聚酰胺的不足之處在于:由于熱膨脹和吸水性所至的尺寸精度不夠,耐酸性差,硬度和彈性模量不夠。經改良以后,也是比較優秀的工程塑料之一。
應用
汽車制造方面
用于制造燃料濾網、燃料過濾器、罐、捕集器、儲油槽、發動機汽缸蓋罩、散熱器水缸、平衡旋轉軸齒輪。也可用在汽車的電器配件、接線柱等。另外,它還可用作驅動、控制部件等。
電器電子工業
可用于制造電飯鍋、電動吸塵器、高頻電子食品加熱器,電器產品的接線柱、開關和電阻器等。
醫療器械儀器
用于醫用輸血管、取血器、輸液器等。PA單絲可做外科手術縫線、假發等;另外,電子打字機的數字旋轉盤、接線柱、傳動齒輪、印刷機的帶式過濾片等。
其它方面
用于制作一次性打火機體、堿性干電池襯墊,摩托車駕駛員的頭盔,辦公機器外殼,辦公用椅的角輪、座和靠背,冰鞋、釣魚線等,PA薄膜氣體阻隔性能優良,而且耐油性、耐低溫沖擊性、耐穿透性好,可用于肉、火腿腸等冷凍食品的包裝。聚酰胺還可棒材和板材,也作齒輪或其它傳動裝置。
上海浩銘塑膠有限公司!本公司承諾,所有產品都是原廠家,原包裝一線獨家營銷!
可提供以下報告:COA(產地證明)SGS(檢測報告)MSDS(成分報告)FDA(食品安全報告)UL黃卡(出口報告)正規發票!歡迎新老客戶來電咨詢:
聯系人:鄧小姐
聯系電話:13917657923
聯系QQ:996152797
聯系郵箱:996152797@qq.com